Detection of the Onset of Necking and Accurate Measurement of Strain Limits of AHSS

2018-10-30 16:22:00
LUQIMENG
Original
2998
Junying Min, Tongji University

John E. Carsley, General Motors Company


A neck is a groove that may develop during plastic deformation that deepens and may lead to fracture during the stamping process.

Onset of necking is defined to be the condition at a neck becomes detectable by tactile or visible sensing of the groove of the neck.


The condition of the onset of necking is important to know because localized necking is an unacceptable manufacturing condition.


The challenge is how to measure the onset of necking without having to measure 100’s of test results over a range of severity in the process of neck formation to find a few tests that are as close as possible to the condition to qualify as at the onset of a neck.


Why is this flawed?
? Result depends on the order of the polynomial.
? Shape of the strain distribution depends on the geometry of the tooling and the blank, and therefore the result of the fit with be affected by this.
? The value might be in the ballpark… it might even be a satisfactory conservative limit, but is that good enough?

Measured strains near fractured edge identified to be within the neck (beyond onset of necking)


Measured strains outside the neck

Correction for Nonlinear Strain Path

Many researchers believe that the DIC recorded strain history can be used to determine onset of necking.


Clearly the record of these strains show an increase in the strain rate as the test approaches fracture.


But strain acceleration also results from inhomogeneous straining, even if a neck does not form.


How does one de-convolute a strain signal from localized neck groove from other factors?


Selected points along the line CD that would
eventually form the neck and later fracture

Fit these points to a circle to determine the curvature





An improved curvature method of detecting the onset of localized necking
in Marciniak tests and its extension to Nakazima tests


Junying Min, Thomas B. Stoughton, John E. Carsley, Jianping Lin
International Journal of Mechanical Sciences, 2017,  123, 238-252


Challenges

Fitting to conditions near
zero curvature.


Add an artificial curve to data to avoid zero.
Solutions
Marciniak and
Nakajima test signals
are different.


Redefine Nakajima surface data to a
spherical coordinate system using radius and
arc length.


Selection of the data to
follow the groove.


A) Expand the analysis to cover the area of the
groove.


B) Adopt the approach proposed by the University of
Waterloo (Warswick, et al.).



Scale of local curvature fit is set to 1.5 times the sheet thickness 

Run the curvature fit from A to B for each frame

Let’s look at what these curvature fits look like in the LAST frame before fracture


Focus on the geometry of the DIC surface data to detect the true onset of necking.


Do not support the ad-hoc strain analyses proposed in Europe and current ISO Standards.


This focus on meaningful measurements will enable us to make wider use of AHSS’s by taking more advantage of their limited ductility through more reliable knowledge of their actual limits.


Write a Comment
Eight minus Five =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 午夜片无码区私人影院 亚洲综合激情另类小说区 9久9久热精品视频在线观看 国产九九99久久99大香伊 亚洲国产精品成人av在线 中文字幕一本性无码 日韩精品一区二区三区中文不卡 国产人妻人伦精品无码麻豆 国产成人一区二区三区app 玩弄少妇的肉体k8经典 精品午夜国产福利观看 果冻传媒剧国产剧情mv在线 麻豆亚洲国产成人精品无码区 波多野结衣av无码久久一区 亚洲国产欧美人成 岛国精品一区免费视频在线观看 亚洲香蕉免费有线视频 亚洲国产婷婷六月丁香 国产成人一区二区三区app 亚洲一区二区色一琪琪 在线精品无码字幕无码av 欧美国产日韩久久mv 免费 黄 色 人成 视频 在 线 久久96热在精品国产高清 久久好在线视频 国产成人亚洲综合网站 青青小草av一区二区三区 亚洲午夜成人精品无码 又黄又爽又猛的视频免费 久久精品国产99久久无毒不卡 国产亚洲精品a在线无码| 国产欧美综合在线观看第十页| 大香网伊人久久综合网2018| 欧洲性久久精品| 国产精品美女久久久m| 九九99无码精品视频在线观看| 亚洲人成网77777亚洲色| 在线无码中文字幕一区| 狠狠色丁香久久婷婷综合蜜芽五月| 经典三级欧美在线播放| 成年午夜免费韩国做受视频|